Technical document

How to set the temperature for precision injection molding

2025-06-24 10:36:04 precision injection molding
In precision injection molding, temperature setting is a core parameter, directly impacting part quality, production efficiency, and material performance. This article concisely explains temperature control essentials, material-specific solutions, and smart technology applications.

1. Core Temperature Control Links

(1) Barrel Temperature

The barrel melts and plasticizes materials, with temperatures set in segments based on material properties:


  • Amorphous Plastics (e.g., ABS, PS)

    • Temperature range: Flow temperature to decomposition temperature.

    • Example: ABS barrel temp: 180–240℃ (feed zone: 180–200℃ for material transport; compression zone: 200–220℃ for plasticization; metering zone: 220–240℃ for melt uniformity).

  • Crystalline Plastics (e.g., PP, PA)

    • Temperature range: Above melting point, below decomposition temperature.

    • Example: PP barrel temp: 190–240℃ (metering zone 20–30℃ higher than feed zone for full melting/crystallization).

    injection mould


For special materials (e.g., glass fiber-reinforced, flame-retardant), increase barrel temp by 5–15℃ to compensate for additive effects.

(2) Nozzle Temperature

The nozzle connects the barrel to the mold. Its temperature is 5–10℃ lower than the barrel’s maximum to prevent drooling (leakage) while avoiding solidification.


  • Example: PET injection: Nozzle temp 270–290℃ (matches barrel temp for continuous high-speed injection).

(3) Mold Temperature

Mold temp affects cooling and part quality, adjusted by material/part design:

injection mould

  • Crystalline Plastics

    • Set between Tg (glass transition temp) and Tm (melting temp) for optimal crystallization.

    • Examples: PA66 mold temp: 80–120℃ (enhances strength/stability); PET mold temp: 120–150℃ (boosts crystallinity, reduces stress).

  • Amorphous Plastics

    • Balances melt flow and surface quality.

    • Examples: PC mold temp: 70–120℃ (prevents defects like silver streaks); PMMA mold temp: 50–80℃ (balances gloss and cycle time).


For thin-walled/complex parts (e.g., phone frames), use zone-specific mold temp control (local heating/cooling) to solve filling/deformation issues.

2. Material-Specific Temperature Schemes

(1) General Engineering Plastics

  • PP

    • Barrel: 190–240℃; Mold: 40–80℃.

    • Adjust mold temp: 60–80℃ for toughness (β-crystals); 40–60℃ for rigidity (α-crystals).

  • PC

    • Barrel: 260–320℃ (high-end PC: 300–320℃); Mold: 70–120℃.

    • Strict temp control (±2℃) to avoid yellowing/silver streaks.

    injection mould


(2) High-Performance Plastics

  • LCP

    • Barrel: 300–350℃ (ultra-high temp LCP: 340–380℃); Mold: 100–150℃.

    • High mold temp ensures crystallization orientation (used for 5G connectors).

  • PEEK

    • Barrel: 360–400℃; Mold: 120–180℃.

    • Requires high-temp mold controllers for aerospace/medical parts (strength/environmental resistance).

3. Smart Technology Upgrades

(1) Intelligent Temperature Control

Modern machines use PID auto-tuning to dynamically adjust heating/cooling (e.g., Haitian, Yizumi). Precision: ±0.5℃ (suits optical lenses, micro connectors).

(2) Zone-Specific Mold Temp Control

3D-printed conformal cooling channels + multi-zone controllers enable precise temp zoning.


  • Example: Automotive radar cover: Local high temp (100–120℃) for complex undercuts; low temp (60–80℃) for edge cooling (reduces warpage by 30%+).

injection mould

(3) Big Data + AI Assistance

Data platforms integrate historical temps/quality data. AI models recommend optimal temp curves.


  • Example: Huawei supplier: AI reduces phone case defects from 5% to 1.2%, shortens cycle time by 15%.

4. Practical Operation Tips

(1) Trial Molding Adjustments

Start with supplier-recommended temps (e.g., PA6: barrel 220–260℃, mold 40–80℃). Adjust by part defects (short shot→increase temp; flash→decrease temp) and record “defect–temp” relationships.

(2) Production Monitoring

Use infrared sensors (mold surface) and melt temp sensors (barrel). Compensate for environmental changes (e.g., seasons) by adjusting mold cooling flow/barrel heating.

injection mould

(3) Troubleshooting

  • Melt Degradation (black streaks/bubbles): Lower barrel temp by 5–10℃ or reduce melt residence time (adjust screw speed).

  • Uneven Cooling (warpage): Check mold cooling channels or use “variable mold temp” (high temp during injection, low temp during packing) for quick solidification.


Precision injection molding temperature setting requires integrating material science, equipment tech, and practice. Smart control, AI, and customized processes enable breakthroughs in miniaturized, high-performance parts—supporting innovation in electronics, automotive, and medical industries.

injection mould

Home
Product
News
Contact
主站蜘蛛池模板: 亚洲 欧美 偷自乱 图片| 亚洲色欲色欲综合网站| 天天做天天爱天天综合网2021 | 挺进邻居丰满少妇的身体| 成人午夜性a级毛片免费| 99精品国产兔费观看久久99| 久久综合亚洲色hezyo国产 | 国产丝袜视频一区二区三区| 国产乱了真实在线观看| 亚洲乱码日产精品bd在线观看| 精品无码久久久久国产手机版| 高清熟女国产一区二区三区| 亚洲熟妇久久精品| 亚洲日韩中文字幕在线播放| 无码人妻精品中文字幕免费东京热| 国产乱人伦av在线麻豆a| 国产成人精品a视频| 欧洲乱码伦视频免费| 久久久久久亚洲精品中文字幕| 国产精品久久久久久久久久免费| 天堂√在线中文官网在线| 亚洲综合av一区二区三区不卡| 亚洲av无码国产一区二区三区| 国产美女被遭强高潮免费网站 | 欧美黑人性暴力猛交喷水黑人巨大| 亚洲日韩亚洲另类激情文学| 九色九九九老阿姨| 中文字幕久久精品一区二区三区| 免费a级毛片无码a∨男男| 日本少妇喷浆| 国产99在线 | 中文| 丰满人妻在公车被猛烈进入电影| 日本护士毛茸茸高潮| 婷婷色香合缴缴情av第三区 | 一本久道久久综合狠狠爱| 日韩精品久久无码人妻中文字幕| 亚洲av永久无码精品秋霞电影影院| 亚洲av成人网站在线观看| 国产午夜精品无码| 亚洲国产精品无码中文字满| 精品无人区一区二区三区在线|