2024-12-09 15:58:53 Appearance of injection moulded parts

1. Flow Marks

Problem

Flow marks result from material's physical properties. The material's flow trace, especially when the filler (including color master) isn't well - dispersed, shows as a visible pattern, like a river's flow, especially in areas with inconsistent thickness.

Solutions

  • Adjust Injection Speed: Use multi - stage injection. For uneven - wall - thickness parts, increase speed in thin - wall areas and decrease in thick - wall areas. For common ABS parts, control filling speed at 30 - 50 mm/s.

  • injection mould

  • Control Mold Temperature: Use a mold temperature controller. Different thermoplastics have different optimal mold temperature ranges. For PP, it's 40 - 60 °C; for PC, 80 - 100 °C. Set temperature sensors inside the mold for real - time monitoring.

  • injection mould

  • Optimize Gate Design: Redesign the gate according to part structure and material. Increase gate size to reduce melt flow rate and choose a proper gate location. For flat parts, a side gate in the middle of the length might be suitable.

2. Tiger Skin Pattern

Problem

The material's physical properties, like in modified automotive plastics with base materials and rubber particles, cause a wavy ejective appearance. Strong - elasticity plastics and color - master coloring issues can also lead to this pattern.

injection mould

Solutions

  • Materials: Strictly control material quality, use the same - batch stable materials and conduct random inspections. Optimize additive use and ensure uniform dispersion.

  • Mold: Optimize the gate by adjusting size and position. Improve the runner by polishing, controlling size, and checking hot - runner heating elements.

  • Injection Molding Process: Stabilize injection parameters, control speed fluctuation within ±5% with closed - loop control. Use a high - precision temperature controller, especially for complex molds with partition temperature control.

3. Trapped Air

Problem

Trapped gas, which differs from gas marks, can't move with the fluid at the end or in corners. Compressed gas raises temperature, causing oxidation and possible burning and yellowing on the product surface. Symptoms include wavy patterns, material shortage, yellowing, and blackening.

Solutions

  • Optimize Exhaust System: Check and clean vent holes and slots. Add an exhaust tank (width 0.02 - 0.05 mm, depth 0.01 - 0.03 mm) in gas - trapping areas. Use ventilated steel for better exhaust.

  • Improve Mold Structure: Simplify complex molds to reduce gas - trapping. Use vacuum exhaust to extract air before injection.

  • injection mould

4. Cold Material

Problem

Cold material forms for two main reasons: the front - end material solidifies in the cycle and is pushed by the back - end material, or there are leftover scraps from the last mold (like shovel - glue leftovers, gate wire - drawing scraps, or electrostatic - adsorbed scraps on the parting surface). This causes an illusion of gas marks on the product surface.

Solutions

  • Adjust Barrel Temperature: Set each barrel section's temperature according to the plastic material. For cold - material - prone materials like nylon (PA), set the starting temperature at 240 - 260 °C. Ensure a proper temperature gradient for uniform heating.

  • Optimize Injection Molding Machine Start - up: Before restarting, pre - plasticize to remelt potential cold - material blocks. Set a preheating program to rotate the screw and increase barrel temperature.

  • Improve Runner System Design: Optimize the flow path by shortening its length and increasing its diameter (e.g., from 3 mm to 4 mm for small parts). Regularly check and maintain hot - runner heating elements.

  • Shorten Injection Cycle: Optimize injection speed and pressure - holding time. Increase injection speed and adjust pressure - holding time to reduce melt residence time in the runner and gate, especially for thin - wall parts.

injection mould


Home
Product
News
Contact
主站蜘蛛池模板: 亚洲欧美日本久久综合网站点击 | 久久婷婷久久一区二区三区| 亚洲高清毛片一区二区| 亚洲 欧美 变态 另类 综合| 中文无码av一区二区三区| 大肉大捧一进一出好爽视频mba| 4444亚洲人成无码网在线观看| 日韩欧美群交p内射捆绑| 亚洲av无码男人的天堂在线| 免费看国产曰批40分钟| 中文字幕一精品亚洲无线一区 | 日韩经典午夜福利发布| 暖暖 免费 高清 日本 在线| 国产熟女乱子视频正在播放| 亚洲国产成人精品无码区宅男?| 五十路亲子中出在线观看| 99精品无人区乱码在线观看 | 国产特级毛片aaaaaa高潮流水| 国内少妇高潮嗷嗷叫在线播放| 国产精品亚洲аv无码播放 | 偷看农村妇女牲交| 无套内谢孕妇毛片免费看| 激情综合亚洲色婷婷五月| 国产精品久久久一区二区三区| 亚洲国产精品热久久| 久久夜色撩人精品国产av| 性欧美video高清| 中文字幕免费不卡二区| 久久精品国产亚洲av麻豆软件| 国产成人无码精品一区不卡| 亚洲处破女av日韩精品| 天堂8中文在线最新版在线| 色哟哟最新在线观看入口| 国产成人精品午夜二三区波多野| 色综合久久久无码中文字幕波多| 国产av天堂无码一区二区三区| 色欲人妻aaaaaa无码| 久久久久亚洲av片无码v| а√最新版在线天堂| 在线涩涩免费观看国产精品| 亚洲国产成人综合精品|